Soft Ferrite Cores
|
Soft
ferrite is a kind of nonmetallic magnetic materials, which is made
up of ferric oxide and other metallic oxides such as MnO, NiO and
ZnO. It has a high resistivity so it's eddy-current loss at high
frequency is much less than that of metallic magnetic materials.
Soft ferrite cores are widely used in computers, tele-communication
equipment, consumer's electronics such as TV, VTR and audio sets,
industrial |
|
|
automation
equipment and various kinds of electronic instruments, etc..
|
MnZn
Power Material----------------------Click here
for shapes
MnZn
High Permeability Material
| |
Characteristics
|
|
UNIT
|
MP3K
|
MP30
|
MP40
|
| |
|
|
3000±25%
|
2500±25%
|
2300±25%
|
| |
Amplitude
Permeability
|
|
3000min
|
3200min
|
3000min
|
| |
Saturation
Flux Density
|
25°C
|
mT
|
470
|
500
|
500
|
| |
100°C
|
mT
|
370
|
390
|
390
|
| |
Remanence
|
25°C
|
mT
|
120
|
110
|
110
|
| |
100°C
|
mT
|
85
|
60
|
55
|
| |
Coercivity
|
25°C
|
A/m
|
12
|
12
|
14
|
| |
100°C
|
A/m
|
7
|
10
|
9
|
| |
Power
Loss
|
|
25°C
|
kW/m3
|
125
|
140
|
105
|
| |
25kHz
|
60°C
|
kW/m3
|
90
|
95
|
75
|
| |
200mT
|
100°C
|
kW/m3
|
125
|
110
|
70
|
| |
|
25°C
|
kW/m3
|
|
700
|
600
|
| |
100kHz
|
60°C
|
kW/m3
|
|
500
|
460
|
| |
200mT
|
100°C
|
kW/m3
|
|
600
|
410
|
| |
|
120°C
|
kW/m3
|
|
|
500
|
| |
Electrical
Resistivity
|
|
W.m
|
6
|
9
|
6
|
| |
Cruie
Temp.
|
|
°C
|
200
|
230
|
215
|
| |
Density
|
|
g/cm3
|
4.8
|
4.8
|
4.8
|
Deflection
Yoke Cores Material
NiZn
Material
| |
Characteristics
|
Unit |
MH5K |
MH7K |
MH7K |
| |
Initial
Permeability (miac)
|
|
5000±25% |
7000±25% |
10000±25% |
| |
Relative
temperature coeffivient (am/miac)
|
x
10-6/°C |
-0.5
~ 2.0
(20~60°C) |
-0.5
~ 2.0
(20~60°C)
|
-0.5
~ 1.5
(20~60°C) |
| |
Relative
loss factor tand/miac(10kHz)
|
x
10-6 |
<6.5
(10kHz)
|
<7(10kHz)
|
<7(10kHz)
|
| |
Disaccommodation
factor DF[1
to 10 minutes]
|
x
10-6 |
<3 |
<2.5 |
2 |
| |
Saturation
flux density Bs [H=1194A/m]
|
mT |
420 |
410 |
400 |
| |
Remanence
Br
|
mT |
140 |
100 |
90 |
| |
Coercivity
Hc
|
A/m |
8 |
7.5 |
7.2 |
| |
Electrical
resistivity r
|
W.m |
1 |
0.3 |
0.15 |
| |
Curie
temperature Tc
|
°C |
>135 |
>125 |
>120 |
| |
Density
d
|
g/m3 |
4.8 |
4.9 |
4.9 |
| |
Characteristics
|
R5
|
R10
|
R100
|
R200
|
R1K
|
R1K5
|
R2K
|
| |
Initial
Permeability mi
|
5+/-20%
|
10+/-20%
|
100+/-20%
|
200+/-20%
|
1000+/-20%
|
1500+/-20%
|
2000+/-20%
|
| |
tand/mix10-6
|
<650
(10MHz)
|
<550
(10MHz)
|
<400
(0.3MHz)
|
<350
(0.3MHz)
|
<15
(0.05MHz)
|
<10
(0.01MHz)
|
<10
(0.01MHz)
|
| |
Bs
(mT)
|
180
|
160
|
300
|
360
|
310
|
320
|
320
|
| |
aFx
10-6/°C (-22°C-55°C)
|
-7~7
|
-40~10
|
15~35
|
25~65
|
1~3
|
3~5
|
2~5
|
| |
Curie
Temp. Tc(°C)
|
420
|
400
|
250
|
200
|
150
|
120
|
120
|
| |
Density
d(g/cm3)
|
4.0
|
4.0
|
4.4
|
4.4
|
4.5
|
4.8
|
4.8
|
| |
Property
|
Symbol
|
Unit
|
R350R
|
R450R
|
R500R
|
R800R
|
| |
AC
initial Permeability(1KHz 0.25mT)
|
mi
|
|
350+/-20%
|
450+/-20%
|
500+/-20%
|
800+/-20%
|
| |
Saturation
Magnetic Flux density
|
Bs
|
mT
|
240
|
250
|
400
|
330
|
| |
Remanence
|
Br
|
mT
|
180
|
160
|
160
|
180
|
| |
Coercive
Factor
|
Hcb
|
A/m
|
<39.8
|
<30
|
<32
|
<40
|
| |
Relative
Loss Force(0.1MHz)
|
tgd/mi
|
x10-6
|
<50
|
<48
|
<40
|
<30
|
| |
Relative Temperature Coefficient 20~80°C
|
amr
|
x10-6
|
<46
|
<46
|
<20
|
<7
|
| |
Curie
temp.
|
Tc
|
°C
|
<150
|
<150
|
<200
|
<150
|
| |
Cut-off
Frequency
|
fc
|
MHz
|
0.5
|
0.5
|
1
|
0.4
|
| |
Relative
Power loss (100mT 16KHz)
|
P
|
mw/g
|
<40
|
38
|
40
|
30
|
|
|
For